HEAT-TREATABLE WROUGHT ALLOY 6060 |
COMMERCIAL DESIGNATION: 6060 STANDARD REF. No(UNI ITALY):9006/1 |
Chemical composition limits in % |
Alloy |
Cu max |
Fe max |
Mg |
Si |
Mn max |
Zn max |
Ti max |
Cr max |
Total impurities except Fe+Ti max |
Al |
Theoretic semis |
- 0,10 |
- 0,35 |
0,45 0,38-0,5 |
0,45 0,38-0,5 |
- 0,1 |
- 0,1 |
0,10 |
0,10 |
- 0,30 |
remainder |
Physical properties |
Density:2,70 kg/dm 3 Melting temperature: 600 °C Specific heat at 100 °C: 0,22 cal/g -1°C-1Thermal conductivity at 20 °C O: 0,42 cal/sec cm °C |
Coefficient of linear expansion: 20 to 100 °C 23 . 10 -6-°C -120 to 200 °C 24 . 10 -6-°C -120 to 300 °C 25 . 10 -6-°C -1Specific electrical resistance at 20 °C: T6:3,25 m W cm Modulus of elasticity: 6700 Kg/mm 2 |
Extrusions |
Type of extrusion |
Description |
Symbol |
Section max mm2 |
Ult. Tensile strenght Kg/mm2 |
Yield point Kg/mm2 |
Elongati-on % |
Brinell hardness HB Kg/mm2 |
any extrusion |
As extruded Heat-treated Heat-treated Heat-treated |
F T1 T5 T6 |
12000 12000 - - - |
12-18 14-18 19-26 21-27 20-26 |
7-12 8-14 15-21 17-23 16-22 |
16-25 16-20 11-18 12-18 12-18 |
30-45 35-50 50-70 60-80 60-80 |